Home/Knowledge/Silane crosslinked PE–rubber compound

Cable compounds · Process & line configuration · 8 min read

Silane Crosslinked PE–Rubber Compound: Processing and KTE-65B Line Configuration

Rubber-modified silane crosslinkable PE is a reactive compound, not a simple blend. Here is the two-step process, a reference formulation, the four-way feeding layout, and the point where strand pelletizing stops working.

This page collects our floor notes on silane crosslinked pe rubber compound: how the line is laid out, the numbers we reference most, and the checks that prevent the usual startup problems.

Quick answer

Silane crosslinked PE–rubber compound is made in two separate steps. First graft a vinylsilane onto PE — optionally with EPDM rubber — using 0.05–0.15 phr peroxide at 150–200 °C. Then blend in a 2–5% tin-catalyst masterbatch and cure the shaped cable or tube in 70–90 °C water or steam. Keep the grafting and the catalyst in separate barrels: mixing them in one extruder causes pre-crosslinking and a blocked machine.

On a KTE-65B, specify L/D 44–48, four-way feeding, vacuum devolatilization and a reference output of 140–200 kg/h. Use water-bath strand pelletizing for hard, PE-rich grades; switch to underwater cutting when the rubber content makes the strand soft and sticky.

2 stepsgraft first, catalyst after — never one barrel
150–200 °Cgrafting window, limits set by silane and peroxide
140–200 kg/hKTE-65 reference, crosslinked PE compound
L/D 44–48catalogue ratio for PE silane crosslinking
KTE-65B twin screw extruder for silane crosslinked PE rubber compound
KTE-65B grafting line for silane crosslinkable PE · Further reading: Wikipedia: Cross-linked polyethylene

Why is this compound made in two steps instead of one?

Silane crosslinking (the Sioplas route) separates the chemical reaction from the shaping operation. The extruder only grafts silane onto the polymer chain. The crosslink — the Si–O–Si network — forms later, after the cable or pipe has been shaped, when moisture activates a tin catalyst. That separation is the whole reason the process is controllable on a standard twin screw.

The grafting reaction is fast: in an optimized industrial extruder, at least 80% of the added silane is grafted within the few minutes of residence time. The resulting granules remain thermoplastic and can be stored and re-processed. Crosslinking is triggered only after the catalyst masterbatch is blended in and the part sees hot water or steam.

Table 1. One-step versus two-step silane crosslinking, and the practical consequence for line design.
RouteHow it runsProcess windowLine consequence
Two-step (Sioplas) — this articleStep 1 grafts silane + peroxide; catalyst masterbatch blended in laterWide — graft and catalyst never meet at melt temperatureOne compounding extruder for the graft; catalyst added by the compounder or at the cable line
One-step (Monosil) — specialtyPE + silane + initiator + catalyst all fed into one high-shear long screwNarrow — gel formation starts if temperature or residence time driftsLonger L/D, tighter dosing, dedicated nitrogen and moisture control; not the default choice

Published process reviews name VTMS (vinyltrimethoxysilane, A-171) as the common grafting monomer; VTES (A-151) hydrolyses more slowly and is chosen where storage stability matters more than cure speed.

What is a reference formulation for rubber-modified silane crosslinked PE?

The numbers below are published patent and supplier ranges, not a production recipe. They are a starting point for a trial. Grafting efficiency, melt index of the PE and the grade of rubber decide the real dosage — confirm each one on your own material.

Table 2. Reference formulation — typical ranges, validate in a pilot trial before production.
ComponentDosageFunctionBasis
LDPE / LLDPE / HDPE carrier100 phrBase resin, grafting substrateVinylsilane grafts to LDPE, LLDPE, HDPE, EVA and EPDM
EPDM / EPM rubber5–20 phrRaises melt viscosity, reduces bubbles from peroxide residueGranted patent US 4,289,860
Vinylsilane (VTMS / VTES)1–4 phrGrafting monomer; later forms the crosslinkSupplier guidance 1–2% (A-151) and 2–4% (VTMS)
DCP peroxide0.05–0.15 phrRadical initiator for the graft reactionSilane supplier processing note
Antioxidant0.2–0.3 phrProtects PE during the high-temperature graft stepCompound practice, grade dependent
Tin catalyst masterbatch2–5% of compoundActivates moisture cure after shapingCommercial silane-crosslinkable EPDM datasheet: 5% for thick sections, 7–10% for small conductors

A patent teaches 0.5–10 parts silane per 100 parts base polymer and warns that DCP has high crosslink efficiency — too much of it crosslinks the PE in the barrel instead of grafting it. A lower-crosslink-efficiency peroxide is preferred where grafting, not C–C crosslinking, is the goal.

The catalyst must stay out of this extruder

The catalyst masterbatch is blended with the grafted granules downstream, or supplied separately to the cable line. If catalyst and silane meet inside a hot barrel, the compound starts to gel in the screw. On a production line that means a full clean-out, not a setpoint adjustment.

How do you set the temperature profile without pre-crosslinking?

There is no single published number. A commercial silane-crosslinkable EPDM cable compound runs a supplier-recommended profile of 130 / 150 / 180 / 190 / 200 °C from feed to die with the screw cooling water at 40–60 °C. Other process references put the grafting reaction zone at 190–210 °C, while a VTMS supplier recommends 150–170 °C for grafting. Treat all of them as starting points and let melt temperature, torque and gel content decide the final ladder.

Table 3. Reference barrel profile for grafting on KTE-65B — starting values, °C.
Zone groupRangeWhat is happeningLimit to watch
Feed (zones 1–2)130–150Solid conveying, no premature meltingBridging if the throat runs hot
Melting (zones 3–5)160–190PE and rubber soften; shear buildsRubber viscosity, motor load
Grafting (zones 6–8)180–200DCP decomposes, silane grafts onto the chainKeep below 210 °C — C–C crosslinking competes with grafting
Vacuum / metering (zones 9–10)180–200Remove unreacted silane and volatile residueVacuum seal before and after the vent
Die190–200Stable melt at the screen pack and die plateNo stagnant pockets where pre-cure can start

The die and head must be stream-lined with no dead spots: a commercial datasheet for crosslinkable EPDM explicitly warns that stagnant material pre-cures. Recommended screen pack is 30/50 mesh (or 600/300 micron).

What does the feeding and devolatilization layout need to look like?

A rubber-modified crosslinkable compound is not a one-hopper job. Four streams have to enter at the right point and at the right accuracy. Small-dose errors matter here because the graft level sets the final crosslink density.

Table 4. Feeding and venting layout on a KTE-65B line.
StreamFeed pointEquipmentWhy
PE pellets (main)Feed throatTwin-screw gravimetric feeder±0.5% accuracy; base resin sets the ratio
EPDM rubberMain or sideSingle-screw feeder; crammer for sheet or low-bulk stockPelletized rubber can join the main feed; sheet bridges in a twin screw
Silane + peroxideAfter meltingLiquid metering pump, jacketed lineLiquid injection after melt; low dose, must be uniform
Tin catalyst masterbatchDownstreamSeparate blender or cable-line feederNever in the grafting barrel
Vacuum devolatilizationZone 9–102.2–3.85 kW vacuum, dual portRemoves unreacted silane and volatile by-products

Gravimetric feeders are selected on the minimum rate, not the maximum: a 1–5 kg/h or 3–15 kg/h range keeps small additive doses accurate. Calibrate at 5 Hz by collecting for one minute and weighing — an uncalibrated feeder is the most common cause of batch-to-batch drift.

What is the KTE-65B line configuration for this material?

The base machine is the same KTE-65B used for TPE/TPR and cable compounds. What changes is the screw configuration, the feeding layout and the pelletizing head. Catalogue data below are reference values, subject to a material trial.

Table 5. KTE-65B configuration for rubber-modified silane crosslinkable PE.
SectionSpecification
Main extruderKTE-65B, screw Ø62.4 mm, 90 kW, 600 rpm, torque 2 × 860 N·m, L/D 44–48
Screw designMelting → dispersive mixing → grafting reaction zone → melt-sealed vacuum zone → low-shear metering; W6Mo5Cr4V2 elements, bimetallic barrel liner
FeedingFour streams per Table 4; gravimetric for PE and small doses, liquid pump for silane/peroxide
Melt filtrationHydraulic screen changer; 30/50 mesh pack; change at 7–10 MPa, never above 20 MPa
Devolatilization2.2–3.85 kW vacuum with reverse-thread melt seals on both sides of the port
Pelletizing — hard gradesWater-bath strand line: cooling bath, air knife, strand cutter
Pelletizing — soft gradesUnderwater unit KUW03: 18 × Ø3.2 mm die holes, 4 kW cutter, centrifugal dewaterer, VS-300 sieve, 1 m³ silo
ControlSiemens PLC, MCGS touchscreen, Delta inverters, Omron temperature control, 0–50 MPa melt pressure
Table 6. Reference output by material on a KTE-65 class machine — catalogue values, confirm by trial.
MaterialReference outputNote
Silane / radiation / chemically crosslinked PE140–200 kg/hReaction control limits throughput
PE + EPDM compound, no crosslinking160–280 kg/hGeneral blend, wider window
TPE / TPR compound on KTE-65B underwater line150–200 kg/hMeasured line configuration, 90 kW / L/D 48:1

Do not quote the general-purpose 200–450 kg/h figure for a reactive crosslinking compound. The catalogue crosslinked-PE row is narrower, and the narrower range governs.

Strand or underwater: which pelletizing method fits this compound?

This is the decision that changes the quotation most. It follows the hardness and tack of the grafted melt, not the name on the datasheet. Soft, rubber-rich or oil-extended grades do not form a strand that survives a water bath; a strand line will show constant breakage and sticking.

Table 7. Pelletizing selection by compound hardness.
GradeIndicative hardnessPelletizingReason
PE-rich, low rubber contentHardWater-bath strand — catalogue defaultStable strands, lowest operating cost; the catalogue default for PE silane crosslinking at L/D 44–48
Medium rubber contentShore A > 90 / Shore D > 42Water-ring hot faceRound pellets, short water contact, works where a strand is marginal
Rubber-rich, soft or oil-extendedShore A ~40 and belowUnderwater — recommendedInstant water quench at the die face stops deformation and sticking; near-spherical pellets, enclosed process

Underwater systems are documented for XLPE cable compounds, MAH grafting, TPE/TPV, EVA and soft elastomers. Typical pellet diameter is 0.8–4.0 mm and surface moisture after the dewaterer is below 0.1% for most standard polymers. Strand cutting is rated poor for elastomers precisely because the strands stick.

A practical rule from the line

If the customer says “rubber + PE + silane” without a hardness or a rubber percentage, ask for both before locking the quote. Low rubber content on PE is a strand job. A soft, tacky elastomer compound is an underwater job. The two lines are not interchangeable, and the price difference is significant.

Three mistakes we see on this compound

  1. Putting catalyst and silane in the same extruder. The compound gels in the barrel and the line has to be stripped. Keep the catalyst masterbatch downstream — that is the entire point of the two-step route.
  2. Quoting a strand line for a soft rubber compound. The strand sticks in the bath and breaks at the cutter. Once the rubber content pushes the melt below roughly Shore A 90, price an underwater unit instead.
  3. Skipping vacuum or using the wrong screen pack. Unreacted silane and peroxide residue stay in the pellet, and bubbles or gel particles appear later in the cable insulation. Use a dual-port vacuum with melt seals and a 30/50 mesh pack.

FAQ

What is the difference between silane and peroxide crosslinking?

Peroxide crosslinking happens inside the extruder at high temperature, in a narrow window between decomposition and scorching. Silane crosslinking separates the steps: the extruder grafts silane onto the chain, and the actual crosslink forms later in hot water or steam (70–90 °C) after the cable or tube is shaped. That is why silane routes are preferred where a conventional extrusion line is already in place.

Can a KTE-65B run the one-step (Monosil) process?

Technically a long-screw, high-shear machine can, but it is not the default. One-step feeding puts PE, silane, initiator and catalyst in the same barrel, so gel formation starts if temperature or residence time drifts. It needs tighter dosing, moisture control and a longer L/D. For most cable compounds the two-step Sioplas route is the more forgiving choice.

What output can a KTE-65B reach on crosslinked PE compound?

Catalogue reference is 140–200 kg/h for silane, radiation or chemically crosslinked PE on a KTE-65 class machine. An underwater TPE/TPR line of the same size is rated 150–200 kg/h. Both are reference values — confirm with a trial using your formulation, because reaction control, not screw volume, sets the ceiling here.

Why add EPDM rubber to silane crosslinked PE?

A granted patent (US 4,289,860) adds 5–20 parts EPDM or EPM per 100 parts of base polymer to raise melt viscosity and reduce bubbles caused by peroxide decomposition residue. Commercial suppliers also sell silane-crosslinkable EPDM compounds directly for flexible low- and medium-voltage cable insulation, so the rubber-containing route is established practice, not an experiment.

What screen pack and die hole size should I use?

A supplier datasheet for silane-crosslinkable EPDM recommends 30/50 mesh (or 600/300 micron) and a streamlined head with no stagnation points. For an underwater head on KTE-65B, the delivered configuration is 18 holes of Ø3.2 mm. Change the screen at 7–10 MPa melt pressure and never exceed 20 MPa.

Should I choose strand or underwater pelletizing?

Choose by the hardness of the grafted melt. Hard, PE-rich grades run on a water-bath strand line at the lowest cost. Grades around Shore A > 90 / Shore D > 42 suit water-ring hot face. Soft, rubber-rich or oil-extended grades below roughly Shore A 40 need underwater cutting — an instant water quench at the die face prevents the pellets from deforming and sticking together.

When does the final crosslinking actually happen?

After shaping. The grafted granules are still thermoplastic; the tin catalyst is blended in at 2–5%, and the finished cable or tube is cured in hot water or low-pressure steam up to about 70 °C (many processes use 60–90 °C, from a few hours to a day or more). Catalyst strength is selected by insulation thickness — stronger catalyst for sections above 1.5 mm, milder catalyst for small conductors such as 1–4 mm².

Sources and method

Formulation ranges come from granted patent US 4,289,860 (silane grafting on thermoplastics and elastomers) and published silane supplier processing notes for VTMS/VTES; the barrel profile, screen pack and catalyst dosage follow a commercial silane-crosslinkable EPDM compound datasheet. Pelletizing selection follows published underwater-pelletizing engineering notes for XLPE and soft elastomers. Machine data, L/D guidance and output ranges are from Kerke catalogue data and a delivered KTE-65B TPE/TPR underwater line. Formulation figures are published ranges, not Kerke recommendations — confirm them with a material trial and with your compound supplier before production.

Silane Crosslinked PE–Rubber Compound — the short version

Related on this site: Silane crosslinked PE cable compound line · Pelletizing methods compared · Feeding and throughput · L/D ratio by material · TPE/TPU/TPR pelletizing · KTE-65B twin screw extruder

Bottom line. Rubber-modified silane crosslinkable PE is a reactive compound, not a simple blend. Use the references above to shortlist, then let the material decide: a 25–50 kg lab trial settles filler ceiling, pellet shape and output before you commit to a line.