Home/Applications/PLA Pelletizing

Application · Biodegradable & PLA

PLA Pelletizing: Temperature Window & Drying

PLA has a 30 °C working window. Ten degrees low and it will not melt homogenously; ten degrees high and molecular weight drops in a step, not a slope. A reference pla pelletizing page from Kerke.

PLA Pelletizing — workshop photo 1, Kerke workshop, NanjingPLA Pelletizing — workshop photo 1, Kerke workshop, Nanjing
PLA Pelletizing — workshop photo 2, Kerke workshop, NanjingPLA Pelletizing — workshop photo 2, Kerke workshop, Nanjing
PLA Pelletizing — workshop photo 3, Kerke workshop, NanjingPLA Pelletizing — workshop photo 3, Kerke workshop, Nanjing
PLA Pelletizing — workshop photo 4, Kerke workshop, NanjingPLA Pelletizing — workshop photo 4, Kerke workshop, Nanjing
PLA Pelletizing — workshop photo 5, Kerke workshop, NanjingPLA Pelletizing — workshop photo 5, Kerke workshop, Nanjing
PLA Pelletizing — workshop photo 6, Kerke workshop, NanjingPLA Pelletizing — workshop photo 6, Kerke workshop, Nanjing
Running video — PLA Pelletizing, Kerke workshop
Running video — PLA Pelletizing, Kerke workshop

Quick answer

PLA compounding and pelletizing needs precise temperature control (140–190 °C), vacuum devolatilization and moisture below 250 ppm to avoid hydrolysis. Output 100–800 kg/h on KTE-50B/65B with air-cooled strand pelletizing.

170–200 °Cprocessing window
80 °C × 4 hdrying
<0.05%moisture

Workshop photos and a running video — shot on our own lines, not stock images.

What sets the limit

PLA is crystallized and dried, metered into a low-shear melt zone, devolatilized, filtered and strand-pelletized with air cooling. Residence time is kept short to protect IV.

Table 1. Key parameters for pla extrusion & pelletizing line. Reference values — confirm on a material trial.
ParameterValue / range
Temperature140–190 °C
Moisture target< 250 ppm after drying
L/D40–44
DevolatilizationVacuum vent, 2 stages for high IV grades
Output (reference)100–800 kg/h
ModelKTE-50B, KTE-65B

Output figures are measured on the reference material stated above. Filler grade, bulk density and moisture move output by ±15% — that is why every quotation we issue is tied to a trial report.

Process flow, step by step

  1. FeedingLoss-in-weight dosing of polymer and filler; side feeder or liquid injection where the formulation needs it.
  2. Melting and dispersingScrew geometry with 45°/90° kneading blocks; barrel profile 140–190 °C.
  3. DevolatilizationVacuum vent at −0.06 to −0.09 MPa removes moisture and volatiles before the die.
  4. Pressure build-upThrottle or discharge section stabilises die pressure; a melt pump where gauge control matters.
  5. Pelletizing and packingdie-face or strand pelletizing, see the pelletizing page; then centrifugal dryer, vibrating screen and bagging.

Equipment configuration

Table 2. What the line is made of, and why each part is specified that way.
StageEquipmentWhy this choice
Main machineCo-Rotating Twin Screw ExtruderArchitecture follows the filling level and the mixing duty, not the required tonnage.
Screw geometryBuilding-block elements, W6Mo5Cr4V2, bimetallic linerWear package for abrasive filler; mixing blocks only where dispersion demands them.
FeedingLoss-in-weight feeder, side feeder where neededRecipe accuracy: ±0.5% short term on the weighed component.
PelletizingPelletizing systemChosen by polymer and filler ceiling — water contact is the deciding column.
DownstreamCentrifugal dryer, vibrating screen, baggingFines below 2% and moisture below the specification of your downstream process.

Output by model

Table 3. Co-rotating twin screw KTE — reference output. Full range on the machine page.
ModelDia. (mm)Speed (rpm)Motor (kW)Torque (N·m)Output (kg/h)
KTE-50B50.5500–60055–752×52580–200
KTE-50D50.5300–80075–902×860100–300
KTE-52B51.4500–60055–752×72080–200
KTE-52D51.4500–60075–1102×1050100–400
KTE-65B62.4500–60090–1102×860200–450
KTE-65D62.4300–800132–1602×1530350–600
KTE-75B71500–600132–1602×1530300–800
KTE-75D71300–800200–3152×2100500–1000
KTE-85B85500–600220–3152×2100550–1000
KTE-95B93500–600250–3152×3000800–1500
KTE-95D93500–800315–5002×48001000–2000
KTE-135B135500–600315–5002×48001500–3000
KTE-135D135500–800500–10002×78001500–4000

Three mistakes that cost the most

1. Skipping crystallization before drying fuses the pellets into a block.

Skipping crystallization before drying fuses the pellets into a block.

2. High shear screws raise melt temperature and drop IV measurably.

High shear screws raise melt temperature and drop IV measurably.

3. Water bath above 25 °C

Water bath above 25 °C — strands embrittle and break, and the pellets start hydrolysing before they reach the bag; hold the bath at 15–25 °C.

FAQ

How much IV loss per pass?

0.02–0.05 dL/g with a properly dried feed and low-shear screw; more than 0.1 means the drying or temperature is wrong.

Can the same line run PBAT?

Yes — PBAT runs at lower temperature and needs a different screw profile, but the platform is the same.

What output can you guarantee for this application?

The reference band is 100–800 kg/h, measured on the stated material. We quote a guaranteed figure only after a trial on your own material, because filler grade, bulk density and moisture move output by ±15%.

Can we run our material before ordering?

Yes — send 25–50 kg. We return pellets, a running video and a report with temperatures, screw speed, feeder settings and output per hour. The trial is free; you cover the freight.

What is the delivery time?

30–45 working days for standard configurations, 45–70 for custom screw geometry and ODM work. Voltage and frequency are built for the destination country.

Where these numbers come from

Parameters are taken from the Kerke product parameter table and the product master data sheet, and cross-checked against commissioning records for lines in the same application. Formulations and temperature windows are typical industry values, not a recommendation for your specific compound — every figure marked reference must be confirmed on a material trial before it becomes a contractual number.

Reviewed by the Kerke process team, Nanjing. Page updated 6 November 2026.

Tell us your material — we will tell you the line

Send 25–50 kg and we run it on our lab extruder: pellets, running video and a capacity report back in 3–7 days.

PLA pelletizing — the short version

Note on pla pelletizing: the numbers above are reference ranges from Kerke's own trial runs, not catalogue promises. Screw geometry, wear package and pelletizing method are set on the trial bench first, so the output you compare is the output you get. If your grade is not in the tables, send it — the closest configuration is usually a change of screw set, not a different machine.

Related on this site: Machine range: KTE-50B to 135D · Pelletizing methods compared · quotation and free trial · Wikipedia: Masterbatch